水性油墨印刷后卷料粘连 Blocking 故障
粘连(set-off)指印刷面在复卷后与料背粘在一起。水性油墨产线的首因是油墨层内残余水分。本指南定位粘连原因并在线修复。
典型故障现象
- 退卷时印刷转移到料背
- 卷内层光泽损失
- 夏季/高湿天气更严重
- 卷芯部(张力最大)更严重
根因排查清单(按优先级)
1. 油墨层残余水分
- Incomplete drying leaves 3-6% water in the ink film. This plasticizes the binder and causes set-off.
- Confirm web temperature at dryer exit reaches 65°C.
2. 复卷张力
- Too high rewind pressure squeezes ink layers together. Tension should be set lower than for solvent runs.
- Taper tension toward roll center to reduce inner-layer pressure.
3. 环境湿度与仓储
- Water-based printed rolls should cool to room temperature before packing. Hot rolls trap moisture inside.
- Store rolls below 60% RH; do not stack them directly on concrete floors.
4. 油墨连接料软化
- If blocking persists after drying, the binder Tg may be too low for the line speed. Discuss with supplier for a higher-Tg grade.
分步解决方案
- 确认烘箱出口膜面温度≥65℃
- 降低复卷张力,卷芯用锥度张力
- 复卷后冷却30分钟再包装
- 仓储20-25℃、湿度<60%RH
- 若仍粘连,改用高Tg快干型号
需要技术支持或样品?
请提供您的基材规格、印刷机参数和故障照片,我们杭州应用工程师将在1个工作日内给出针对性建议并安排实验室样品。
发送技术咨询 申请样品常见问题
为什么水性油墨比溶剂型更容易粘连?
水蒸发更慢;干燥不充分时残余水分软化连接料,卷料反粘。
加蜡能解决粘连吗?
蜡改善表面滑爽,但不能替代充分干燥;与提高烘箱风量配合使用。
印刷卷料应放置多久后加工?
在受控湿度下静置24-48小时再复合或分切。